Waddywood

Waddywood (Acacia peuce)
Waddywood (Acacia peuce)

Common Name(s): Waddywood, Waddi

Scientific Name: Acacia peuce

Distribution: Simpson Desert, Australia

Tree Size: 50-60 ft (15-18 m) tall,

                 ~1 ft (.3 m) trunk diameter

Average Dried Weight: 89 lbs/ft3 (1430 kg/m3)

Specific Gravity (Basic, 12% MC): 1.16, 1.43

Janka Hardness: 4,630 lbf (20,600 N)

Modulus of Rupture: 21,750 lbf/in2 (150.0 MPa)*

Elastic Modulus: 3,118,000 lbf/in2 (21.50 GPa)*

Crushing Strength: 12,450 lbf/in2 (80.0 MPa)*

*Provisional strength group values based on density, derived from AS/NZS 2878:2000

Shrinkage: No data available

Color/Appearance: Heartwood is dark reddish or purplish brown, sometimes nearly black. The sharply demarcated sapwood is light yellow.

Grain/Texture: Grain is straight, with a uniform, medium texture.

Rot Resistance: Given its past use as fence posts, the wood is assumed to be very durable.

Workability: Difficult to work with hand or machine tools due to its extremely high density. Reportedly turns and finishes well.

Odor: No characteristic odor.

Allergies/Toxicity: Besides the standard health risks associated with any type of wood dust, no further health reactions have been associated with Waddywood (though this may be due to the rarity of the tree itself). See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Pricing/Availability: A rare (and protected) desert tree with no commercial presence.

Sustainability: This wood species is not listed in the CITES Appendices or on the IUCN Red List of Threatened Species. However, it is a protected species listed as vulnerable under Australia’s Environment Protection and Biodiversity Conservation Act.

Common Uses: Clubs, turned objects, carvings, and other small decorative purposes.

Comments: The common name is said to be of aboriginal origin, where natives would make “waddies”—heavy wooden clubs—from the wood.

When the tree is younger, its growth form resembles that of a conifer (such as a pine tree), and its species name, peuce, is derived from the Greek work for pine. After several decades of growth, mature trees finally begin to take on their adult form and branch out from the main trunk.

Images: Drag the slider up/down to toggle between raw and finished wood.

[caption id="attachment_22101" align="alignleft" width="300"]Waddywood (Acacia peuce) Waddywood (Acacia peuce)[/caption]

Identification: See the article on Hardwood Anatomy for definitions of endgrain features.

Waddywood (endgrain 10x)
Waddywood (endgrain 10x)
Waddywood (endgrain 1x)
Waddywood (endgrain 1x)

Porosity: diffuse porous

Arrangement: solitary and radial multiples

Vessels: small to medium, moderately numerous to numerous; amber to reddish brown deposits common

Parenchyma: vasicentric, lozenge, confluent, and banded

Rays: narrow to medium width, normal spacing

Lookalikes/Substitutes: May be confused with gidgee (Acacia cambagei) or pink gidgee (A. crombiei) based on very dark purplish heartwood, high density, and heartwood fluorescence. Waddywood will generally have more extensive (confluent) parenchyma and slightly smaller pores.

Notes: Heartwood fluoresces under blacklight.

Related Content:

Subscribe
Notify of
guest


4 Comments
Inline Feedbacks
View all comments
Jeff S

Hello Eric, a few years back I received a couple of older pieces labeled Purple Gidgee. I was 99% sure they were Pink Gidgee as they did have the pink band that forms between the heart wood & sap. The band does fade over time. The wood when cut is brownish & turns dark purple when exposed to sun light. Although I think it’s pink gidgee Im not entirely sure it isn’t Waddy wood. I sent a few pics of a sample. I’m not sure it’s enough to make a identification but I thought you may be able to tell… Read more »

AE0C5DD9-45F4-4C49-9D3C-351369E71A50.jpeg
7083CA6E-1196-47A2-9871-3EF712112550.jpeg
12BB24F9-B397-4078-B84E-71C397A82A07.jpeg
9ED99EE5-58E9-4BAD-93D0-68154F5B78D9.jpeg
Jeff S

Thank you for the reply! Being that the two are so similar I thought that there might be a tell in the end grains. Beautiful wood regardless! Thanks for takin a look!

Johan Jonasson

Hello. So this is the hardest wood that you have ever encountered?