Balau

Light Red Meranti (Shorea spp.)
Balau (Shorea spp.)

View More Images Below

Common Name(s): Balau

Scientific Name: Shorea spp.

Distribution: Southeast Asia

Tree Size: 150-200 ft (45-60 m) tall, 3-6 ft (1-2 m) trunk diameter

Average Dried Weight: 53 lbs/ft3 (850 kg/m3)

Specific Gravity (Basic, 12% MC): .69, .85

Janka Hardness: 1,600 lbf (7,120 N)

Modulus of Rupture: 17,730 lbf/in2 (122.3 MPa)

Elastic Modulus: 2,457,000 lbf/in2 (16.95 GPa)

Crushing Strength: 10,280 lbf/in2 (70.9 MPa)

Shrinkage: Radial: 5.5%, Tangential: 10.1%, Volumetric: 15.7%, T/R Ratio: 1.8

Color/Appearance: Color can be highly variable depending upon the species: ranging from a pale straw color, to a darker reddish brown.

Grain/Texture: Has a coarse texture with medium to large pores. Grain is sometimes interlocked.

Rot Resistance: Highly variable among species; should be considered as non-durable in regard to decay resistance, and is also susceptible to insect attack.

Workability: Typically hard to work, due to its high density. Some species may have a slight blunting effect on tools due to small levels of silica present in the wood. Glues, stains, and finishes well.

Odor: No characteristic odor.

Allergies/Toxicity: Although severe reactions are quite uncommon, Balau in the Shorea genus has been reported to cause eye, throat, and skin irritation. See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Pricing/Availability: Balau is widely harvested and widely available worldwide. It should be moderately priced despite the fact that it is imported.

Sustainability: Balau is not listed in the CITES Appendices, but many species in the Shorea genus are on the IUCN Red List. The majority of Shorea species are listed as being critically endangered due to a population reduction of over 80% in the past three generations, caused by a decline in its natural range, and exploitation.

Common Uses: Plywood,veneer, general construction, flooring, as well as a number of other general utility purposes.

Comments: Sometimes referred to as “Lauan,” wood in the Shorea genus is very commonly used in southeast Asia, and there is an abundance of variety between the difference species: each with different working properties, appearances, and mechanical strength values.

The five main groupings for Meranti (Lauan) are: Light Red Meranti, Dark Red Meranti, White Meranti, Yellow Meranti, and Balau. The strength and mechanical values listed at the top of this page represent the average of a handful of species within the corresponding group.

Also called Philippine Mahogany, Meranti bears no relation to  what is considered to be “true” mahogany in the Swietenia and Khaya genera.

Related Species:

Related Articles:

Scans/Pictures: There are currently no pictures of this exact wood species, but a similar species within the Shorea genus is being substituted (Light Red Meranti). If you’d like to contribute a wood sample of this specific species to be scanned, (even small pieces of veneer can be sent), please use the contact form.

Light Red Meranti (Shorea spp.)
Light Red Meranti (sanded)
Light Red Meranti (sealed)
Light Red Meranti (sealed)
   
Subscribe
Notify of
guest
28 Comments
Inline Feedbacks
View all comments
James

I am looking for information on “Yellow Balau,” which is sold here in the Pacific Northwest, but not listed separately on WDB..
Is it the same as Balau?
How does it compare to Cumaru in appearance?
Would it be compatible with Cumaru in a deck project?
Thank you very much.
James in Seattle

Bret

Also – I got some old stuff from a guy that had been in his backyard raw for 15 years. It was a bit cracked and splintered but easily cleaned up with a planer. The endgrain shows tightly packed pores filled with tyloses – seemingly quite water resistant.

The only issue is not being certain what you’re actually getting as all of the Shorea species can look similar but lack similar characteristics.

Pedro

Hi our decking is warped can red balau be sanded? If so what grade of sandpaper can we use?

Toto

Hi Pedro, you can sand them using 120 grit, then finish up with 240 grit sandpaper. Apply teak oil afterwards to preserve the glow of the wood. Reapply every 3 months or as frequently as needed.

Rasheed

I want to use Balau for outdoor decking in UAE, any advice?

Ting

One of the most suitable wood for outdoor decking. However the question is how to you make sure you are getting the genuine Balau timber not other imitation timber?

William

Could you use this wood to make a bookcase indoors?

David Simon

CYRUS.Thanks for the information, 4 Yorkshire sliding sashes made of yellow balau, should they be wood preserved before oiling? North Lincolnshire England thanks dave.

Jacques Hauray

I have serious doubt about the durability of Red Balau. It is basically a meranti or lauan which are used primarily as veneer for plywood. It is not a class 1 wood but class 3 which is not recommended for outdoor use.. It is kinda of a shame that distributors of Red Lauan represents this wood as durable.

Bert Prinsloo

I have a balau deck around my pool.Over the years(approx.5 years) the deck has dried out and splintered.It is very dangerous if you walk on it bare feet.Any suggestions how i can solve the peoblem?

Xxxvv

Do some sanding, apply another layers of coating will do. Can last for another 5 years

Lim more seen

Use alkyd urethane wood coating to seal the wood. If you want to preserve the wood colour, select a clear coating. Sand the deck with 240 grid sand paper and apply linseed oil as required before sealing the the deck.

Willem Louw

Get a industrial belt sander and sand your deck

Paul Caponetti

Hey everyone. I had some Red Balau (from Batu, sold as decking material) that I made into an end grain cutting board. The whole process was an experiment, but the product came out really awesome. Does anyone know if Red Balau is safe to put food on after I do the normal cutting board things (wash, condition, oil, etc)?

Dias

This is not from batu, but country origin is indonesian, nova (america) was bough from here, so many type woods like this, such as bangkirai,

Yudi Eko Santosa

comment image
Bangkirai / Yellow Balau

Maya

what is the other alternative for red balau? Can i use red meranti?

Wooden Decking Durban

Hi Maya. In South Africa we get largely yellow balau which is of good quality. What we get here that is called red balau is inferior quality. I’ve used it a few times in outdoor wooden decks here in Durban and it is more porous and softer than our yellow balau. https://blog.thewoodjoint.co.za

kah22

I’m looking at a patio set described as a Jakarta Wooden Patio Set

Is Jakarta a region where this wood is grown or is it the actual wood?

J J

I am haing some cracking in some doors i made with a yellow balau core and a 1/8″ thick face veneer of yellow balau. The faces are cracking lengthwise. Why would this happen to kiln dried wood

Wooden Decking Durban

Hi JJ. Balau is a very oily and resinous wood so even though it has been kiln dried it still contains a fair amount of resins and oils. As this dries out over time it can cause cracking especially in such a thin veneer. Possibly also because the veneer is stuck to the carcass of the door it is prohibited from expanding and contracting. I’ve noticed a fair amount of expansion and contraction in balau. I made T & G floor boards which didn’t work well as they contracted quite a lot after we installed them. Balau doesn’t like to… Read more »

I wouldn’t coat it with anything. Coatings can peel and flake, oil can’t. http://blog.thewoodjoint.co.za

Jason Anicich

does the bacteria and do the insects this wood is prized by live in north America? It seems to me the climate change could preclude your assertions? can anyone in the US confirm having a rotten or insect eaten red balau deck?

tim

I don’t get it, they are saying Red Balau is the same as Philippine mahogany or Luan. I started my young life as a boat builder and I know my woods and I have bought lots of Luan but this stuff is nothing like luan at all, first off it’s ten times as dense. You can drive nails through luan, but this stuff forget it. You must drill every hole. It’s an entirely different wood.

donald

can I coat balau wood with poly

Cyrus

to preserve the natural wood grains, I recommend using linseed oil, teak oil or mineral oil instead because this is a very tough and durable wood and unless you are dealing with very harsh conditions, there is no need to take away some of its natural beauties by using polyurethane, use oils instead, otherwise you can use poly on anything

Lim more seen

Depends on the appearance and the use of your wood. If you are exposing to water frequently, poly is a good solution