Wood Identification Guide

Wood Identification Guide

by Eric Meier

When attempting to identify a wood sample, it’s important to keep in mind the limitations and obstacles that are present in our task. Before starting, please have a look at The Truth Behind Wood Identification to approach the task in a proper mindset; I consider the linked article to be required reading for all those visiting my site with the intent of identifying wood.

1. Confirm it is actually solid wood.

Before proceeding too much farther into the remaining steps, it’s first necessary to confirm that the material in question is actually a solid piece of wood, and not a man-made composite or piece of plastic made to imitate wood.

A solid piece of Cocobolo: note how the grain naturally wraps around the sides and endgrain of the wood.

Can you see the end-grain? 

Manufactured wood such as MDF, OSB, and particleboard all have a distinct look that is—in nearly all cases—easily distinguishable from the endgrain of real wood. Look for growth rings—formed by the yearly growth of a tree—which will be a dead-giveaway that the wood sample in question is a solid, genuine chunk of wood taken from a tree.

Viewing the end of this “board” reveals its true identity: particleboard.

Is it veneered? 

If you see a large panel that has a repeating grain pattern, it may be a veneer. In such cases, a very thin layer of real wood is peeled from a tree and attached to a substrate; sometimes the veneer can be one continuous repeating piece because it is rotary-sliced to shave off the veneer layer as the tree trunk is spun by machines. Assuming it is a real wood veneer with a distinct grain and texture—and not merely a piece of printed plastic—you may still be able to identify the outer veneer wood in question, but you should still realize that is it only a veneer and not a solid piece of wood.

Large repeating patterns suggest a veneer.

Is it painted or printed to look like wood? 

Many times, especially on medium to large-sized flat panels for furniture, a piece of particleboard or MDF is either laminated with a piece of wood-colored plastic, or simply painted to look like wood grain. Many of today’s interior hardwood flooring planks are good examples of these pseudo-wood products: they are essentially a man-made material made of sawdust, glues, resins, and durable plastics.

2. Look at the color.

Some questions to immediately ask yourself:

Is the color of the wood natural, or is it stained?

If there is even a chance that the color isn’t natural, the odds are increased that the entire effort of identifying the wood will be in vain.

The reddish brown stain used on this piece of Jatoba (Hymenaea courbaril) has been planed away on top, exposing the paler color of the raw wood underneath.

Is it weathered or have a patina?

Many woods, when left outside in the elements, tend to turn a bland gray color. Also, even interior wood also takes on a patina as it ages: some woods get darker, or redder, and some even get lighter or lose their color; but for the most part, wood tends to darken with age.

Fresh sanding near the end of this Osage Orange (Maclura pomifera) board has exposed the characteristic yellow coloration of the wood, which has a strong tendency to shift down to a golden brown over time.

Is it possible to sand or plane the board to see the natural raw color of the wood?

The most predictable baseline to use when identifying wood is in a freshly sanded state. This eliminates the chances of a stain or natural aging skewing the color diagnosis of the wood.

3. Observe the wood grain.

If the wood is unfinished, then look at the texture of the grain. Ask yourself these questions:

Does the wood have an open, porous texture?

Most softwoods will be almost perfectly smooth with no grain indentations, while many common hardwoods have an open pore structure, such as oak or mahogany; though there are some hardwoods that are also smooth to the touch, such as maple.

Can you tell if the wood is quartersawn or plainsawn?

By observing the grain patterns, many times you can tell how the board was cut from the tree. Some wood species have dramatically different grain patterns from plainsawn to quartersawn surfaces. For instance, on their quartersawn surfaces, lacewood has large lace patterns, oak has flecks, and maple has the characteristic “butcher block” appearance.

Is there any figure or unusual characteristics, such as sapwood, curly or wild grain, burl/knots, etc.?

Some species of wood have figure that is much more common than in other species: for example, curly figure is fairly common in soft maple, and the curls are usually well-pronounced and close together. Yet when birch or cherry has a curly grain, it is more often much less pronounced, and the curls are spaced farther apart.

Curly Maple (sealed)
The strong, tight curl seen in this wood sample is very characteristic of Maple (Acer spp.).

4. Consider the weight and hardness of the wood.

If it’s possible, pick the piece of wood up and get a sense of its weight, and compare it to other known wood species. Try gouging the edge with your fingernail to get a sense of its hardness. If you have a scale, you can take measurements of the length, width, and thickness of the wood, and combine them to find the density of the wood. This can be helpful to compare to other density readings found in the database. When examining the wood in question, compare it to other known wood species, and ask yourself these questions:

Is the wood dry?

Wood from freshly felled trees, or wood that has been stored in an extremely humid environment will have very high moisture contents. In some freshly sawn pieces, moisture could account for over half of the wood’s total weight! Likewise, wood that has been stored in extremely dry conditions of less than 25% relative humidity will most likely feel lighter than average.

How does the wood’s weight compare to other species?

Taking into account the size of the board, how does its weight compare to other benchmark woods? Is it heavier than oak? Is it lighter than pine? Look at the weight numbers for a few wood species that are close to yours, and get a ballpark estimate of its weight.

A piece of Lignum Vitae is weighed on a small digital scale.

How hard is the wood? 

Obviously softwoods will tend to be softer than hardwoods, but try to get a sense of how it compares to other known woods. Density and hardness are closely related, so if the wood is heavy, it will most likely be hard too. If the wood is a part of a finished item that you can’t adequately weigh, you might be able to test the hardness by gouging it in an inconspicuous area. Also, if it is used in a piece of furniture, such as a tabletop, a general idea of its hardness can be assessed by the number and depth of the gouges/dings in the piece given its age and use. A tabletop made of pine will have much deeper dents than a tabletop made of Oak. Additionally, you can always try the “fingernail test” as a rough hardness indicator:  find a crisp edge of the wood, and with your fingernail try to push in as hard as you can and see if you’re able to make a dent in the wood.

5. Consider its history.

Many times we forget common sense and logic when attempting to identify wood. If you’ve got a piece of Amish furniture from Pennsylvania, chances are more likely that the wood  will be made of something like black walnut or cherry, and not African wenge or jatoba. You might call it “wood profiling,” but sometimes it can pay to be a little prejudiced when it comes to wood identification. Some common-sense questions to ask yourself when trying to identify a piece of wood:

Where did it come from?

Knowing as much as you can about the source of the wood—even the smallest details—can be helpful. If the wood came from a wood pile or a lumber mill where all the pieces were from trees processed locally, then the potential species are immediately limited. If the wood came from a builder of antique furniture, or a boat-builder, or a trim carpenter: each of these occupations will tend to use certain species of woods much more often than others, making a logical guess much simpler.

Despite its discoloration and wear, it’s very likely that this rolling pin is made of hard maple.

How old is it?

As with the wood’s source, its age will also help in identification purposes. Not only will it help to determine if the wood should have developed a natural patina, but it will also suggest certain species which were more prevalent at different times in history. For instance, many acoustic guitars made before the 1990s have featured Brazilian rosewood backs/sides, yet due to CITES restrictions placed upon that species, East Indian rosewood became a much more common species on newer guitars. (And this is a continuing shift as newer replacements are sought for rosewoods altogether.)

How large is the piece of wood?

Some species of trees are typically very small—some are even considered shrubs—while others get quite large. For instance, if you see a large panel or section of wood that’s entirely black, chances are it’s either painted, dyed, or stained: Gaboon ebony and related species are typically very small and very expensive.

What is the wood’s intended use?

Simply knowing what the wood was intended for—when considered in conjunction with where it came from and how old it is—can give you many clues to help identify it. In some applications, certain wood species are used much more frequently than others, so that you can make an educated guess as to the species of the wood based upon the application where it was used. For instance, in the United States: many older houses with solid hardwood floors have commonly used either red oak or hard maple; many antique furniture pieces have featured quartersawn white oak; many violins have spruce tops; many closet items used aromatic red cedar, and so forth. While it’s not a 100% guarantee, “profiling” the wood in question will help reduce the number of possible suspects, and aid in deducing the correct species.

6. Find the X-Factor.

Sometimes, after all the normal characteristics of a sample have been considered, the identity of the wood in question is still not apparent. In these instances—particularly in situations where a sample has been narrowed down to only a few possible remaining choices—it’s sometimes helpful to bring in specialized tests and other narrower means of identification.

The following techniques and recommendations don’t necessarily have a wide application in initially sorting out wood species and eliminating large swaths of wood species, but will most likely be of use only as a final step in special identification circumstances.

Odor

Believe it or not, freshly machined wood can have a very identifiable scent. When your eyes and hands can’t quite get a definitive answer, sometimes your nose can. Assuming there is no stain, finish, or preservative on or in the wood, quickly sand, saw, or otherwise machine a section of the wood in question, and take a whiff of the aroma.

Although new scents can be very difficult to express in words, many times the scent of an unknown wood may be similar to other known scents. For instance, rosewoods (Dalbergia spp.) are so named for their characteristic odor that is reminiscent of roses. Although difficult to directly communicate, with enough firsthand experience scents can become a memorable and powerful means of wood identification.

Fluorescence

While certain woods can appear basically identical to one another under normal lighting conditions, when exposed to certain wavelengths—such as those found in blacklights—the wood will absorb and emit light in a different (visible) wavelength. This phenomenon is known as fluorescence, and certain woods can be distinguished by the presence or absence of their fluorescent qualities. See the article Fluorescence: A Secret Weapon in Wood Identification for more information.

Black Locust: fluorescence (under blacklight)
Black Locust (Robinia pseudoacacia) glows a bright yellow-green when placed under a blacklight.

Chemical Testing

There are only a small number of chemical tests regularly used on wood, most of which are very specialized and were developed to help distinguish easily confused species with one another. They work by detecting differences in the composition of heartwood extractives. A chemical substance (called a reagent) is usually dissolved in water and applied to the wood surface: the surface is then observed for any type of chemical reaction (and accompanying color change) that may occur. Two of the most useful are the tests that are meant to separate Red and White Oak, and Red and Hard Maple.

Heartwood Extractives Leachability

Sometimes a wood species will have heartwood extractives that will be readily leachable in water and capable of conspicuously tinting a solution of water a specific color. For instance, the heartwood extractives contained in osage orange (Maclura pomifera) contain a yellowish-brown dye that is soluble in water. (This can sometimes be observed anecdotally when the wood is glued with a water-based adhesive: the glue’s squeeze-out is an unusually vibrant yellow.)

In a simple water extract color test, wood shavings are mixed with water in a vial, test tube, or other suitably small container, and the color of the water is observed after a few minutes. If the heartwood extractives are leachable by water, then a corresponding color change should quickly occur.

In addition to osage orange (Maclura pomifera)merbau (Intsia spp.), and rengas (Gluta spp. and Melanorrhoea spp.) are also noted for their readily leachable heartwood extractives. Because this property is quite uncommon, it can serve to quickly differentiate these woods from other lookalikes.

7. Look at the endgrain.

Perhaps no other technique for accurate identification of wood is as helpful and conclusive as the magnified examination of the endgrain. Frequently, it brings the identification process from a mostly intuitive, unscientific process into a predictable, repeatable, and reliable procedure.

Looking at the endgrain with a magnifier shouldn’t be a mystifying or esoteric art. In many cases, it’s nearly as simple as examining small newsprint under a magnifying glass. There are three components necessary to reap the full benefits contained in the endgrain:

I. A prepared surface.

When working with wood in most capacities, it becomes quickly apparent that endgrain surfaces are not nearly as cooperative or as easily worked as face grain surfaces. However, in this case, it is absolutely critical that a clear and refined endgrain surface is obtained.

For a quick glance of a softwood sample, a very sharp knife or razor blade can be used to take a fresh slice from the endgrain. However, in many denser species, especially in tropical hardwoods, one of the best ways to obtain a clear endgrain view is through diligent sanding. It’s usually best to begin with a relatively smooth saw cut (as from a fine-toothed miter saw blade) and proceed through the grits, starting at around 100, and working up to at least 220 or 320 grit, preferably higher for the cleanest view.

II. The right magnifier.

It need not be expensive, but whatever tool is used to view the endgrain should have adequate magnifying power. In most instances, 10x magnification is ideal, however, anything within the range of 8 to 15x magnification should be suitable for endgrain viewing. (Standard magnifying glasses are typically in the range of 2 to 4x magnification.)

These stronger magnifiers, sometimes called loupes, usually have a smaller viewing area than standard magnifying glasses. Fancier models—with built in lights, or larger viewing surfaces—are available at a premium; but the most basic models are usually only a few dollars.

amazon-button
amazon-button

III. A trained eye.

The third element that constitutes a proper endgrain examination is simply knowing what to look for. In analyzing the patterns, colors, shapes, and spacing of the various anatomical features, there is a veritable storehouse of information within the endgrain—all waiting to be unlocked. Yet, if these elements have not been pointed out and learned, the array of features will simply seem like an unintelligible jumble. The discipline of recognizing anatomical endgrain features is not easily summed up in a few sentences or even a few paragraphs, but it is nonetheless critical to the identification process. To this end, an in-depth look should be given to the various categories, divisions, and elements that constitute endgrain wood identification on the macroscopic level. (In this regard, macroscopic denotes what can be seen with a low-powered, 10x hand lens—without the aid of a microscope—rather than simply what can be seen with the naked eye.) Because the anatomy between softwoods and hardwoods is so divergent, each will be considered and examined separately:

Still stumped?

If you have a mysterious piece of wood that you’d like identified, you’ve got a few options for next steps:

USDA’s Forest Products Laboratory

You can mail your physical wood samples to the Center for Wood Anatomy Research

Pros:

  • Free
  • Professional wood identification

Cons:

  • Only available to US citizens
  • Slow turnaround times (up to a month or more)
  • Limited to three IDs per year

See their Wood ID Factsheet for more info.

Alden Identification Service

You can mail your physical wood samples (even small sections taken from antiques) to Alden Identification Service.

Pros:

  • Professional wood identification
  • Faster turnaround times (ranging from a few days to a week or two)

Cons:

  • Paid service

See their ordering page for more info. (Note that Harry Alden has written several books while at USDA, including both Hardwoods and Softwoods of North America.)

Ask for help online

If the wood ID is merely a curiosity, or non-critical, you can post pictures of the wood in question.

Pros:

  • Free
  • No need to send physical samples

Cons:

  • Greatly limited by the quality of the pictures provided
  • Extra work usually required to get adequate clarity in photos

See article of Common US Hardwoods to help find the most commonly used woods.

Get the hard copy

wood-book-standupIf you’re interested in getting all that makes The Wood Database unique distilled into a single, real-world resource, there’s the book that’s based on the website—the Amazon.com best-seller, WOOD! Identifying and Using Hundreds of Woods Worldwide. It contains many of the most popular articles found on this website, as well as hundreds of wood profiles—laid out with the same clarity and convenience of the website—packaged in a shop-friendly hardcover book.
Subscribe
Notify of
guest
4.2K Comments
Inline Feedbacks
View all comments
ben

It was an $80 barn find. I could probably get $1000+ for it when it is all done, but will hold on to it for my future grand children. Original, unrestored & in fair to good condition these go for an easy $2000 to $20,000 depending on model & maker. (Tom Blake is the quintessential designer of these days & though this is missing the plug (or emblem), it is likely either made by one of 3 companies he licensed to reproduce his designs, or a good copy of one of his patents) P.S. Thanks for the expert advice. Look… Read more »

Ted

So this is a 1920’s surf board? Sweeeeet.
That’s way before the Hawaiian influence on WWII vets and the California wave craze.
I’m thinking Antiques Roadshow, that baby’s GOT to be worth some cashola.

ben

I think I may have possibly located the actual model (so possibly actually from the 40’s) see attached (though this one was made of redwood there were a few different companies manufacturing Tom Blake’s designs in those days)

ben

Thank you so much. Here is the before photo, & I will be posting the after later. (p.s. looks like it was later turned to a lifeguard board with a faint “lifeguard blue” paint still visible. I am restoring it to what I think was it’s previous condition (hopefully). This would probably be a “Bordeaux” dark reddish brown as which was traditional in that day….

Ted

Ben – 1st photo looks like yellow pine rotary cut plywood veneer, or possibly fir, 2nd photo looks like a regular fir or hemlock board, but could be pine also. It’s got a lot of age going for it. Good closeup, though. Now I want to see what the whole thing looks like, even if that sounds kooky.

ben

….also here is the tail block which would be neat to identify as well. Thanks.

ben

I am restoring a 1920’s hollow surf/paddle board (called a kook box). Am attaching a picture of the veneer (or early plywood) which I am trying to identify & fix a missing section of the board. Thanks. (GREAT SITE)

Lara

Ted,

I believe the mirror used to sit on top of a sideboard/buffet, and it would have been mounted with the shelf on the top and mirror underneath. I’ve done some research, and the piece dates back to around the 1890’s and early 1900’s. I wish I could have seen the sideboard it was originally made to go with. Thanks so much for your input!

Ted

John, I’m going to guess at Pecan. Lara, Hard to see, but I’m going to guess quarter sawn oak with a dark walnut stain. The 3rd photo, the 1×3 at the bottom(?) looks like QSO & so does the veneer on the left of the same photo. 1st photo, top left, looks like oak there, too. This piece has seen some hard use. Is this a shelf with a mirror under it? Hard to determine it’s purpose. 2nd photo, the veneer on the scrollwork looks like QSO, that the craftsman put there (where it was highly visible) to accentuate the… Read more »

Lara

And here is a third showing more grain patterns….

Lara

Here is another angle of the first photo….

Lara

I’m trying to identify what kind of wood my antique mirror may be. It’s a very heavy piece, and the veneer is starting to peel. I can see wood grain underneath where it has peeled already. I have more photos I can post as well. Thank you!

El

Thanks Eric. Here is a pic of the unfinished, underside of the table. It looks a lot like the Black or Tropical walnut.

Ted

Lisa, Fungus (or …Fungi, if you want to be technical)

El

Hey all. I am trying to ID the top of this dining table (which appears to be a wood veneer).

This photo is of the top.

Lisa

This tree was knocked down 8 years ago and just cut it to move it. What is this strange orange red color?

Nate

What I have found is the case with any “exotic hardwood” is that you always need to be VERY CAREFUL to apply a very controlled amount of force when using ANY “sharp woodworking tools”. In other words NEVER apply excess pressure to ANY part of any grain of “exotic wood”. Many people say, “Whatever, I know what I’m doing…” but I say, “Don’t say I didn’t warn you if you lose a finger, arm and/or leg if you weren’t careful…”

Ted

Marion, you’re too far away to make a species identification. Do you people even read earlier posts? I can’t identify era or style, not my forte.. looks “new” rather than antique, or it’s something that has been stripped down and completely refinished. Pretty shiny for an antique, looks like a gloss polyurethane finish on it. To my taste it would look nicer just plain wood and fluted columns, and without the fruity & leafy thing on the 3rd drawer. That’s hideous. Let me think about that, no, it wouldn’t even look good on the 4th drawer, either. Chintz. Over-embellishment. You… Read more »

Marion barrasso

Inherited bedroom set over 100 yrs old photo of dresser, also vanity desk dresser and bed. Can you tell me what type of wood and style this is’
What era would this be?

Ted

James,
Re17th, maybe lignum vitae?
Re27th, modern post-1950s mass produced, machine made, secondary wood on outside frame, like basswood, cherry veneer with maple inlay. Saw cut around edge is modern innovation to pass off mass produced furniture as “expensive” inlay work. (just think what would grow down in there after little Jimmy spills his frosted cocobomb cereal…EEEEK!)

James

what kind of wood and what era might this be?

James

Anyone know what type of wood this is its a dark very hard type of wood.

Ted

If the rest of you vote to kick me off of here, I’ll understand, and my mother used to say, “if you don’t have something nice to say, don’t say anything” – but I can’t resist.

Mike – Hey, what’s with the blurry photo of firewood?

mike

my freind took these peices out of a boat house/dancehall built i think in the early 1900’s near alexandrea bay new york.

Johan

Eric:
That sounds like a good idea. I’ll repost my last post at the FB page.

Johan

Thank you all for great expertise. The thing I liked so much about this small piece of wood I found, apart from it’s beauty, was how well and how easy it was to get a really high finish to it. I mostly use oil such as “minwax antique oil finish” or “liberon finishing oil” (both are oils mixed with varnish). The wood is also easy to shape with a sander at the same time as it’s quite hard and will withstand both use and abuse. Is this also the caracteristics of pear, cherry and apple wood? What other woods have… Read more »

Ted

Johan, The v-grooves in the ends of your logs are chainsaw marks. I’d say cherry also, based on the graining, and the colors you’re experiencing. Definitely a fruit or nut wood. It is NOT maple. Maple is very light. Maybe walnut or pecan, we need a bark expert to chime in. Cherry darkens over time, but starts out medium brown to dark brown with red hints. The really RED cherry that we see in the US is a stain used habitually by furniture manufacturers so that the public perception is that a species of wood looks that red, when it… Read more »

Johan

I’ve been out sanding the end grain and taken some new pictures. I put a math on the endgrain to help determine size. I’ve also read up on different woods types here on the database and managed to rule out some that I had suspected. I wish I could weigh the piece but I don’t have a scale nor a moisture meter. Conclusions so far: The wood is heavy although very dry. It has dense grain. It sands to a almost gloss finish, endgrain sands to gloss. Doessen’t smell. Has some wavy patterning and dark streaks. Colour is medium reddish… Read more »

Bill

Johan, color and bark, looks like cherry wood. The knot makes it prettier, but it looks like cherry…

Johan

I found this 3″ x 9″ x 18″ piece of wood in a dumpster when i was collecting firewood. I would like to know what it is so that i can get more because this wood is absolutelly fantastic to work with! It sands to an almost shiny surface so there’s almost no open pores. It darkens quite a bit when I apply Liberon finishing oil, wich it soaks up fast, especially at the end grain. It’s quite heavy even though it’s been dried inside for over 2 years now. The sawdust has a orange colour and the cut surface… Read more »

Mark

Eric, I see what you mean. The pores are less packed on your example, which is an awesome high resolution scan.

Mark

Endgrain shot

Mark

One more request if I may.

Can someone confirm if this is sassafras wood. I salvaged this wood from an old dresser that looks like it was built in the 70-80s. I think its sassafras because it has a sweet smell when I cut it and the pores in the endgrain appear to match with your database example.

Mark

I think the weight just gave it away. I was thinking it was African Mahogany after looking through your database, but I think the weight just confirmed it, at least I hope. I had to find an online density calculator and put the measurements of a piece that measured 3″x38″x1.125″ with a weight of 3.23 lbs. The resulting calculation is 43.54 lbs/ft3. The wood to my knowledge has been stored for years in an old garage workshop in Houston which may be the cause of the smell, but it is certianly more prominate once I cleaned it up on the… Read more »

Ted

Mark,

Mahogany

Mark

Here is a shot of the endgrain.

Mark

Fisrt of all great site!

I live in Texas and recently received some old wood from my wife’s grandfather. I am unsure as to the species, and aside from the attached pictures it has a musty smell and contains sap. Any help is greatly appreciated.

Rich

Hi Ted,
The table is very heavy and so are the chairs. Thanks for your comments I guess I will label it as ebony.

Ted

Benny- the bookend matched pieces around the moulding under the top may be rosewood, but the top itself looks like mahogany to me, without the cherry red stain most pieces have, mahogany is a middle brown color like what you have. Walnut doesn’t have the zig-zaggy stripes your piece shows in the 2nd photo bottom center & right. Mahogany does. Pieter – I can’t even guess from the photos you’ve posted. Neat little corner unit, looks like someone has used it hard from the dings on the top surface in the 2nd photo. Maybe a refinisher could tell you what… Read more »