Pink Ivory

Pink Ivory (Berchemia zeyheri)
Pink Ivory (Berchemia zeyheri)

View More Images Below

Common Name(s): Pink Ivory, Red Ivorywood

Scientific Name: Berchemia zeyheri

Distribution: Southern Africa

Tree Size: 100-130 ft (30-40 m) tall, 3-5 ft (1-1.5 m) trunk diameter

Average Dried Weight: 65 lbs/ft3 (1,035 kg/m3)

Specific Gravity (Basic, 12% MC): .90, 1.04

Janka Hardness: 3,230 lbf (14,370 N)

Modulus of Rupture: 20,020 lbf/in2 (138.1 MPa)

Elastic Modulus: 2,193,000 lbf/in2 (15.12 GPa)

Crushing Strength: 11,630 lbf/in2 (80.2 MPa)

Shrinkage: Radial: 4.8%, Tangential: 7.2%, Volumetric: 12.1%, T/R Ratio: 1.5

Color/Appearance: Pink Ivory ranges in color from a pale brownish pink, to a bright, almost neon pink, to a deep red. Typically the most valuable pieces of Pink Ivory are a vibrant  pink. Pink Ivory can commonly be seen with a curly or fiddleback grain pattern, further enhancing its visual impact. Sapwood of Pink Ivory tends to be pale yellow to light brown, with a somewhat gradual demarcation from heartwood. Color changes in Pink Ivory (becoming faded or dull over time) can be problematic and are not fully understood.

Grain/Texture: Grain is straight to interlocked; fine, even texture with good natural luster.

Endgrain: Diffuse-porous; medium pores in no specific arrangement, nuymerous; commonly in radial multiples of 2-4; gum/heartwood deposits common, though not easily seen with lens; growth rings may be distinct due to increased pore frequency in earlywood; narrow to medium rays visible without lens; parenchyma not visible with lens.

Rot Resistance: Rated as durable to very durable regarding decay resistance, Pink Ivory is said to have excellent weathering characteristics: though it is seldom used in applications where this would be an issue.

Workability: Pink Ivory has a pronounced blunting effect on cutting edges, and it’s fairly difficult to work in board form. Tearout can occur on figured or quartersawn sections during planing. Pink Ivory is much more common in applications involving carving or turning, and it turns and finishes well.

Odor: Pink Ivory has a distinct and somewhat unpleasant odor when being worked.

Allergies/Toxicity: Besides the standard health risks associated with any type of wood dust, no further health reactions have been associated with Pink Ivory. See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Pricing/Availability: Reputed to be a scarce commodity, Pink Ivory is typically very expensive, usually on par with Gaboon Ebony: another pricey African import.

Sustainability: This wood species is not listed in the CITES Appendices or on the IUCN Red List of Threatened Species.

Common Uses: Carving, veneers, inlay, knife handles, billiard cues, chessmen, and other turned objects.

Comments: Pink Ivory trees are said to be both rare and valuable, and have been rumored to be “rarer than diamonds.” Other reports state that the tree is relatively common in some areas of South Africa—though large trees with straight, defect-free trunks are much more scarce. According to folklore, the tree is considered sacred to the Zulus in South Africa and is reserved for royalty.

Related Species:

None available.

Related Articles:

Scans/Pictures: The bright pink/red colors shown below represent what is usually the most sought-after hues of Pink Ivory. Also, you’ll see some Pink Ivory that has been turned into an ice cream scoop handle, and has been used in the Neapolitan pattern consisting of Black Walnut (chocolate), Hard Maple (vanilla), and Pink Ivory (strawberry).

Pink Ivory (sanded)
Pink Ivory (sanded)
Pink Ivory (sealed)
Pink Ivory (sealed)
Pink Ivory (endgrain)
Pink Ivory (endgrain)
Pink Ivory (endgrain 10x)
Pink Ivory (endgrain 10x)
Pink Ivory (turned)
Pink Ivory (turned)
 

[iframe id=”https://www.youtube.com/embed/UvHEBMTv1aY?rel=0″]

Subscribe
Notify of
guest
65 Comments
Inline Feedbacks
View all comments
Mike Trihorns

Hello, not sure if the author is still around to answer questions but does anyone know how fast the color turns brown?

Mike Stafford

A box in Pink Ivory

IMG_1503-mod-Custom
Anthony

I was very fortunate in collecting a very old Stump used as a barricade in the gardens of our small community near Bela Bela, South Africa. It was very heavy indeed, I didn’t know what it was either. I soon found out that it was not going to be easy to saw down the middle of it by hand. I Had to find someone nearby to make the cut for me, so I did, only to have him tell me a few weeks later, after he managed to slice through, that he never experienced wood that hard in his life.… Read more »

IMG-20230810-WA0016.jpg
IMG-20230810-WA0015.jpg
Collage_20230905_153912.jpg
Collage_20230905_154112.jpg
Matt

Is it possible to bend pink ivory?

Chris

Yes. If it is thin enough. 1/8 and 1/16 veneer bends easily

Jay

Hey guys, can you help me please.

I was wondering how long it takes to grow this tree from a seed to a size that can be used for wood?

Mike Premo

I had a fallen tree that I cut and noticed the beautiful inner color of the tree. Found another one growing on our property. Wondered what kind of tree it might be and the closest I could find is pink ivory, but the tree & bark look quite different. What do you think? Pink ivory or some other species?

20230115_133340.jpg
20230115_134957.jpg
20230115_133820.jpg
20230115_133823.jpg
Mike Premo

Yes, I asked another friend who does cabinetry and he confirmed eastern red cedar also!

I didn’t notice any odor when cutting, but it had maybe been dead for a while.

Filip

Yestern red cedar for sure (Juniperus virginiana). Very good and important wood for making blocks in recorders. It has very nice and strong – like perfume- fragrance.

Last edited 3 years ago by Filip
sven

A turned bowl from pink ivory

177.jpg
Erdei Dávid

Helloo!
Can someone help me unfortunately I couldn’t find any information about the brown ivory. I would be interested in its hardness and how it is related to pink ivory. thanks for the help.I want to make a wind instrument. :)

Loren Javernick

Talk about dulling effect. I sharpened my chisel before turning this and by the time I knocked the corners off I had to sharpen again because the wood kept wanting to catch fire. Honestly it was pretty difficult to turn compared to desert ironwood and African Blackwood, the latter of which is an absolute dreamboat on the lathe despite being harder than pink ivory. It says here that it doesn’t have any known health effects but I would be careful about the dust; I only breathed it in once and it made me sneeze a bunch and my nose all… Read more »

image.jpg
Patrick Brennan

I had the same experience (janka 3230 !!!). This wood forced a switch to the Robert Sorby Turnmaster (one tool, 3 interchangeable carbide tips) – yes you need a diamond- coated “credit card” to sharpen them, but it’s EASY. Those carbide cutters went through the pink ivory with no difficulty – what a pleasure.

Hope this helps !

Pete

I turned some ivorywood for the first time today but will avoid it in future. It really was hard work, took a long time and dulled my tools very quickly. I then sanded it on the lathe with only the dust extractor on but forgot my mask, and must have inhaled some dust which has left me with a headache and feeling a little nauseous. The finished piece looks superb but I didn’t enjoy working with it and will choose some easier wood for my next project.

Ryan

I may have a few large pieces of this, it’s so pink I thought maybe it had been dyed/sprayed pink! Is this in fact pink ivory?

Ryan

Here it is;

A16DB773-F21D-4A85-9A30-6BFCF9526776.jpeg
Patrick Brennan

I’ve bought a fair bit of pink ivory, and hate to disagree with Eric, but your wood looks exactly like many photos of pink ivory offered by Cook Woods, and others. The pink color can be VIBRANT – unfortunately it fades quite a bit to brown over time, and I’ve never found a solution to that.

Patrick Brennan

I understand- how might he determine this, definitively, given that wood’s value ?

Joseph

How about lightly sanding or planing a small section of it to see if the colour gets more vibrant or disappears?

Filip

I have very similar in colour pieces of … old pear wood.

Kevin Kempton

The wood does take a high polish with very fine sandpaper but will darken with age to more of a reddish brown.
I found a large bole at a garage sale. It had a lot of checking and had to take about an inch off all around. I filled the checks with several applications of thin cyanoacrylate and that worked well. Nice smell when working.

P2150872.JPG
Jeff mead

Very cool wood carving you’ve done there.

Filip

Great Sculpture!

Leahcim Samoht

Hello, It’s a beautiful carving you have there but the (above) description for this wood, Pink Ivory, states that it ought to have an unpleasant odor while working with it. Also, your example is awfully red (not in an awful sense… to the contrary, it’s, seemingly, a perfect & HIGHLY desirable red color). I believe there is a chance you are working with some type rosewood…. or, padauk because of the sheer redness of it. Personally, I love working with padauk because of its sweet, almost cinnamon+nutmeg-like aroma. Also, I could be wrong. However, my experience, here, with the “‘database”… Read more »

Gonzalo

Hi Erick,
I have this sample that was thought to be B. zeyheri but I am wondering if it may actually be B. discolor (brown ivory). the end grain is similar (I do not have a proven pink ivory sample to compare though). As you can see in the sample it is not pink and this has been sanded (it is also finished with coats of blonde shellac. The end grain has also been finished but you might be able to see the anatomical features

B. zey.jpg
micro.jpg
Gonzalo

I do not recall any scent when sanding.
The sample stands at 0,91 g/cm3 (MC unknown)

Rohan

. Mmmmm, Does look VERY simular to Dalbergia Nitidula (Purplewood flat bean) when oxidised.

Robin

I’m sanding down a couple of chairs and they are light pink; hence the reason I googled this wood color. Should I not paint them? Is the wood worth something?

Berke

Hello .I am in Turkey. I have such a tree. Is this tree pink ivory?

20210512_175127.jpg
20210512_175109.jpg
Berke

Hi.I have polished new photos.The tree is as heavy as iron. Compared to a tree of the same size. unknown wood 0.61 lb , lignum vitea 0.49 Ib.

20210516_175326.jpg
20210516_175228.jpg
Screenshot_20210516-180230_WhatsApp.jpg
Berke

This tree was imported from south africa I know it has been kept dry for about 20 to 30 years.And lignum vitea 20 to 30 years.The dryness levels are the same.I have one of this unknown wood.Lignum vitea I have 160 pieces.It was a reserved material for the yacht.

Berke

yes translation error :) ‘wood’ . yes someone can know in south africa

Rohan

And oh ja! I am from that place South Africa……. In that case, then i am quite “almost certain”, you sir have purple wood flat bean right there. Small shrub, true rosewood, and it doesnt really give of a overwhelming sweet scent when working with it.
Flower of Zimbabwe!

Rohan

Its actually quite wide spread in Africa…… Also called Zebra wood in West Africa, Nigeria and many other names.

Rohan

I know my camera work is a bit crappy, but it does look very similar to Dalbergia Nitidula……will search for some decent photos
.

FB_IMG_1625697639679.jpg
FB_IMG_1625697636306.jpg
FB_IMG_1625697632752.jpg
FB_IMG_1625697639679.jpg
Berke

Unknown wood

20210516_175235.jpg
Lyndon

Bubinga.

Noppadon

Really???!!! Is it true this wood species is not listed in the CITES Appendices or on the IUCN Red List of Threatened Species?
I need to confirm this formation please.

Billy Adams

I have made a beautiful large coffee table, mirror and TV cupboard from a red ivory tree stamp dropped by someone in my yard because it was in their way. Had the stump cut up in planks. Definitely a wood worthy of being called a royal wood, more beautiful than polished iron wood and rivals tamboti.

Robert Flowers

I am having limited success growing Berchemia zeyheri from seed in Southern Arizona. At 5 years old, the bottom 6 inches is only as thick as a broom handle, and will only be sapwood for about 20 years. At 4 years, it produced its first flowers and viable seeds. It does not like frost, but will probably stand the desert winters once it is old enough to have thick bark. Ground squirrels gnaw the bark off saplings..I have been keeping them potted, and bringing indoors through the winters. It keeps its leaves over the winter indoors..

Jon Ugalde

Thank you for your information, I find it very interesting. Can you explain a bit more what does frost make to these trees?

ROSA JIMENEZ

That was so awesome and is the 1st time I’ve ever seen that Wood in my life; it is beautiful, glorious thank you for sharing and for being so kind in your explanation of the Wood.

Bob Gorman

Hello Robert: I tried for years to get Berchemia zeyheri to germinate, using different “drastic” methods which included even using petri dishes with the hard shells carved down to reveal the embryos. However, I did get them to begin to germinate, but they died before really sprouting. I have a friend who lives in Thailand, and he tends to be almost negligent and reckless in the way in which he approaches things. So, I sent him some of B.zeyheri and B.discolor seeds (Which I have never been able to get to germinate.). So, upon arrival at his home in Thailand… Read more »

Oziane

Olá Bob, moro no Estado de Rondônia, Brasil. Há três anos e meio adquiri uma muda da berchemia zeheri de um site chamado Planta Mundo . Meu interesse é variar o pomar. Pelo q li a frutinha é gostosa. Poderia me descrever o sabor da frutinha? A minha está com cerca de 2metros de altura.

Ferrice

Can I have some seeds of Berchemia zeheri ? Would you like to trade or exchange some seeds from South East Asia.

Fyl

Portland is too vastly different from Thailand…. closest you’ll get in USA will probably be Florida, and even then it might be hopeless

Brandon Borrillo

Made a comb out of this wood recently. Sanded the surface up to 2000 grit, the surface feels like glass, and looks fantastic even without a finishing coat. Definitely tricky to cut thin slices of this wood without getting a “tear-out” as mentioned. I broke a tooth on the comb but super glue fixed this seamlessly -probably because the wood is very dense and hard.

Jeffery Brooke

Love working with Pink Ivory, just made a pen/stylus combo for my daughter about 2 hours ago. So far I have only turned Pink Ivory so I have no experience in working with it other than turning. Given the dimensions Pink Ivory is generally available in, inlays, turning or carving is about all it is suitable for. I not only like the look of Pink Ivory, it has a really good feel to it when it’s nicely polished up.

Mike

Just turned some Pink Ivory on the lathe. Turns beautifully; tight, dense grain that polishes well. The shavings and spindle were the color bubble gum, pencil eraser or Pepto-Bismol.

Daniel Ewers

Not experienced with this wood, wanted to make a tobacco pipe from a piece, have heard some woods are toxic in this regard, was hoping for some information. Thanks Dan

Robert Flowers

Toxicity should be minimal, as the color is derived from tannin. The density should help it from charring thru like softer woods, but you might have to be clever and line it with a briarwood dowel, bored out.

Alex

It’s probably not as harmful as what’s being smoked, should be ok.

Nate

I have worked with this wood and it is a ***** to work with…
The grain is very sharp and pointy and interlocked… This wood can bend in small sliver live crazy. It is the most non-straight grain to work with ever!!! Fair warning: Ammonia will bleach the pink color out of this wood…

Ernie Gordon

If you want to see a masterpiece, do a search on Amazon for Dennis Capplinger’s Gospel Banjo book. The banjo on the cover has a solid pink ivory wood neck, and the resonator is maple with pink ivory veneer on top. Quite striking. The neck wood came from Eisenbrand Exotic Hardwoods back when Art was in charge; the veneer was from Certainly Wood. It sounds as awesome as it looks.