Koto (Pterygota macrocarpa)
Koto (Pterygota macrocarpa)

View More Images Below

Common Name(s): Koto

Scientific Name: Pterygota macrocarpa

Distribution: West Africa

Tree Size: 65-100 ft (20-30 m) tall, 2-4 ft (.6-1.2 m) trunk diameter

Average Dried Weight: 37 lbs/ft3 (595 kg/m3)

Specific Gravity (Basic, 12% MC): .51, .59

Janka Hardness: 940 lbf (4,200 N)

Modulus of Rupture: 15,290 lbf/in2 (105.4 MPa)

Elastic Modulus: 1,752,000 lbf/in2 (12.08 GPa)

Crushing Strength: 7,590 lbf/in2 (52.4 MPa)

Shrinkage: Radial: 5.1%, Tangential: 10.6%, Volumetric: 15.0%, T/R Ratio: 2.1

Color/Appearance: Pale yellow heartwood; little color variation from sapwood to heartwood. Quartersawn surfaces can exhibit ray fleck. Steamed or dyed veneer is not uncommon.

Grain/Texture: Straight to slightly interlocked. Texture moderately coarse.

Endgrain: Diffuse-porous; solitary and radial multiples; large pores in no specific arrangement, very few; mineral/gum deposits occasionally present; parenchyma vasicentric, diffuse-in-aggregates, banded; medium to wide rays, spacing wide.

Rot Resistance: Rated as non-durable; poor insect resistance.

Workability: Good working characteristics, though tearout can result on pieces that have interlocked grain. Glues, stains, and finishes well.

Odor: Has a strongly unpleasant smell when green which disappears once dry.

Allergies/Toxicity: Although severe reactions are quite uncommon, Koto has been reported to cause skin irritation. See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Pricing/Availability: Generally available as veneer, prices are in the mid range for an imported hardwood.

Sustainability: This wood species is not listed in the CITES Appendices, but is on the IUCN Red List. It is listed as vulnerable due to a population reduction of over 20% in the past three generations, caused by a decline in its natural range, and exploitation.

Common Uses: Veneer, plywood, and furniture.

Comments: No data available.

Related Species:

None available.

Related Articles:

Scans/Pictures: A special thanks to Steve Earis for providing the wood sample of this wood species.

Koto (Pterygota macrocarpa)
Koto (sanded)

Koto (sealed)
Koto (sealed)

Koto (endgrain)
Koto (endgrain)

Koto (endgrain 10x)
Koto (endgrain 10x)

Koto (gray veneer)
Koto (gray veneer)
Subscribe
Notify of
guest
4 Comments
Inline Feedbacks
View all comments
LRS

I turned a large segmented vase with Koto and found it cut and sanded quite nicely but has open grain like Wenge. It dose not bend well unless cut very thin and then it could be a crap shoot. Ash bends the best of all woods I have used providing it is also cut very thin. I purchased my Koto from Cook Woods in Klamath Falls, Oregon. Give them a call or email, I am sure they will answer all questions.

Dana

I’m wondering about grain comparison between ash and koto. Want a finer grain. Definitely do not want it to be mistaken for oak. Which would be better? Thank you.

LRS

Koto will definitely not be mistaken for oak of any species. It is not as hard as oak and turns nice with sharp tools. The wood has open grain so it takes a lot of finish to get a nice smooth feel to the end product.

Cct

Curious – what would be similar to Koto here in Pacific Northwest – Washington to be exact – in terms of viability, flexibility/bending when working with the wood. Something similar? Most comparable? Thank you