Alaska Paper Birch

Alaska Paper Birch (Betula neoalaskana)
Alaska Paper Birch (Betula neoalaskana)

View More Images Below

Common Name(s): Alaska Paper Birch

Scientific Name: Betula neoalaskana

Distribution: Alaska and northern Canada

Tree Size: 50-65 ft (15-20 m) tall, 1-2 ft (.3-.6 m) trunk diameter

Average Dried Weight: 38 lbs/ft3 (610 kg/m3)

Specific Gravity (Basic, 12% MC): .49, .61

Janka Hardness: 830 lbf (3,690 N)

Modulus of Rupture: 13,600 lbf/in2 (93.8 MPa)

Elastic Modulus: 1,900,000 lbf/in2 (13.10 GPa)

Crushing Strength: 7,450 lbf/in2 (51.4 MPa)

Shrinkage: Radial: 6.5%, Tangential: 9.9%, Volumetric: 16.7%, T/R Ratio: 1.5

Color/Appearance: Heartwood tends to be a light reddish brown, with nearly white sapwood. Occasionally figured pieces are available with a wide, shallow curl similar to the curl found in Cherry. There is virtually no color distinction between annual growth rings, giving Birch a somewhat dull, uniform appearance.

Grain/Texture: Grain is generally straight or slightly wavy. Pores are closed, with a fine, even texture

Rot Resistance: Birch is perishable, and will readily rot and decay if exposed to the elements. The wood is also susceptible to insect attack.

Workability: Generally easy to work with hand and machine tools, though boards with wild grain can cause grain tearout during machining operations. Turns, glues, and finishes well.

Odor: No characteristic odor.

Allergies/Toxicity: Birch in the Betula genus has been reported as a sensitizer. Usually most common reactions simply include skin and respiratory irritation. See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Pricing/Availability: Likely to be rather economical in most instances. Figured boards can be more expensive, but normally plain birch lumber is in the same price range as maple or oak.

Sustainability: This wood species is not listed in the CITES Appendices or on the IUCN Red List of Threatened Species.

Common Uses: Plywood, boxes, crates, turned objects, interior trim, and other small specialty wood items.

Comments: Birch is one of the most widely used woods for veneer and plywood worldwide. Besides regular sheets of plywood, Birch veneer is also used for doors, furniture, and paneling.

Related Species:

Scans/Pictures: There are currently no pictures of this exact wood species, but a similar species within the Betula genus is being substituted (B. alleghaniensis). If you’d like to contribute a wood sample of this specific species to be scanned, (even small pieces of veneer can be sent), please use the contact form.

Yellow Birch (sanded)
Yellow Birch (sanded)

Yellow Birch (sealed)
Yellow Birch (sealed)
Subscribe
Notify of
guest
1 Comment
Inline Feedbacks
View all comments
Neil

In Alaska it’s very popular for bowl turning and spoon carving. It’s food safe and often finished with Walnut Oil or similar. I have made some excellent wooden arrows with it for my recurve and it will stay straight if you can find some straight grained lumber and air dry it completely. It carves well although it takes some hand strength if you use a knife and the wood is dry. Birch stains and dyes poorly resulting in a blotchy look unless you seal it first. AK Paper Birch is probably the hardest and strongest wood that grows in Alaska.