by Eric Meier
In the world of acoustic guitars, perhaps no other tonewood holds the same respect and downright mystique as Brazilian Rosewood (Dalbergia nigra). Yet paradoxically, the wood has been virtually loved to death: since 1992, it’s been on the CITES Appendix I, the most restrictive category of endangered species, (even finished products may not cross international borders). Because of these protective measures, several substitutes have been used in recent years, primarily East Indian Rosewood (Dalbergia latifolia). Hence, for a multitude of reasons, differentiating between true Brazilian Rosewood and many of its close cousins can be very useful.
Brazilian Rosewood |
vs |
East Indian Rosewood |
![]() |
![]() |
|
| Color: Tends to be more variegated, and more on the reddish side. (Can also exhibit a figure in the grain similar to Ziricote that is known as “spider-webbing.” | Color: Tends to be a dark chocolate or purplish brown. | |
| Average Weight: 52 lbs/ft3 (835 kg/m3) The two weights are so close, for all intents and purposes, density is identical. | Average Weight: 52 lbs/ft3 (830 kg/m3) The two weights are so close, for all intents and purposes, density is identical. | |
| Scent: Has a distinct, rose-like scent when being worked. | Scent: Has a distinct, rose-like scent when being worked; some find its scent less pleasant than other Dalbergia rosewoods. | |
![]() |
![]() |
Endgrain: Pay close attention to the endgrain, as it’s one of the best ways to separate the two woods. Each sample above represents approximately a 3/8″ square section of endgrain. The key is in the pore density: East Indian Rosewood has about twice as many pores per square inch as Brazilian Rosewood. This can be difficult to gauge if you don’t have any known samples to compare, but Brazilian Rosewood should have fairly sparsely spaced pores, while East Indian Rosewood should be almost riddled with pores.
Another Useful Trick
Apart from the very characteristic odor, (which should roughly separate it from most non-Dalbergia species), Brazilian Rosewood has another characteristic that can be leveraged in order to help distinguish it from other rosewoods: its heartwood extractives are not water soluble, and will not fluoresce under a blacklight.
Before you get scared off from performing this test, be aware that with a simple blacklight bulb available in any hardware store for only a few dollars, and a few minutes of your time, you can perform both water extract fluorescence and ethanol extract fluorescence tests at home!
For suspected samples of Brazilian Rosewood, take a small test tube or other small transparent container and fill it with some shavings, (a handplane works great for this), and then fill the remainder of the container with water and shake it up for a few seconds. Bring the container under the blacklight and observe the results: true Brazilian Rosewood (Dalbergia nigra) will not fluoresce or show any appreciable change of color under the blacklight, while most other rosewoods will glow a pale blue/green color.
Telling Brazilian Rosewood apart from other common substitutes:
Non-Dalbergias: Use scent to rule out most non-Dalbergia species. (Scents are difficult to describe in words, but certainly no scent at all would be a negative sign.)
East Indian Rosewood: Pore density; water extract fluorescence
Amazon Rosewood: Density—Amazon Rosewood tends to sink in water; water extract fluorescence
Madagascar Rosewood: Water extract fluorescence
Cocobolo: Density—Cocobolo tends to sink in water; water extract fluorescence
Kingwood: Density—Kingwood tends to sink in water; pore size—Kingwood’s pores tend to be smaller; water extract fluorescence
Honduran Rosewood: Density—Honduran Rosewood may not sink in water, but it is roughly 20% heavier; pore size—Honduran Rosewood has slightly varying sizes of pores (ranging from medium-small to large); water extract fluorescence
Are you an aspiring wood nerd?
The poster, Worldwide Woods, Ranked by Hardness, should be required reading for anyone enrolled in the school of wood nerdery. I have amassed over 500 wood species on a single poster, arranged into eight major geographic regions, with each wood sorted and ranked according to its Janka hardness. Each wood has been meticulously documented and photographed, listed with its Janka hardness value (in lbf) and geographic and global hardness rankings. Consider this: the venerable Red Oak (Quercus rubra) sits at only #33 in North America and #278 worldwide for hardness! Aspiring wood nerds be advised: your syllabus may be calling for Worldwide Woods as part of your next assignment!




Hello, could anyone, please, give me some help at identifying this wood? I am torn between Brazilian and Madagascar rosewood. I tried to ask AI, but it was quite uncertain as well, just a bit more inclined to Brazilian.
Some more photos including the bridge and interior
This is my newly acquired 1986 Lowden L32pp (prototype designation) SN#264 after production moved back to Northern Ireland. Based upon poor density I am fairly certain the bridge is Brazilian, the back and sides still are undetermined. It smells wonderful, especially after it warms up from my playing for a few minutes, any input would be appreciated. The ruler marks on the bridge end grain are .5mm. Interior photos show it unfinished.
P.S.
more pics of the cutting board..
possibly goncalo alves or curupay
Bought this cutting board (in local market/gas station/restaurant complex in southern Brazil 2023) cheap but I couldn’t resist the reddish color.. As I’m using it as cutting board I’m not putting oil to recover the look. I was always wondering what tree it came from. Now after I’ve read this article..the reddish color.. I’m wondering if anybody has clue what it could be? I doubt its Brazilian Rosewood.. so I don’t even think that fluorescence test is necessary.. But I’d love to hear your opinion..
Cheers!
Hi, is there a way to test Brazilian Rosewood without taking a wood sample? I have a guitar that Melbourne University hands on viewed for a report . In this report it states by the most senior specialist that he was “loath to take a sample from such a fine instrument.” He stated he couldn’t 100 verify it as Brazilian Rosewood without a sample from it. Is it at all possible to test in another manner that you would be aware of please? This guitar is made, by the very famous Hascal B Halie , Dated, July-20-1973. A am situated… Read more »
May I please get help identifying this rosewood species?
appears to be Brazilian