Honduran Mahogany (Swietenia macrophylla)

Cuban Mahogany (S. macrophylla pictured)

View More Images Below

Common Name(s): Cuban Mahogany, West Indies Mahogany

Scientific Name: Swietenia mahogani

Distribution: Southern Florida and the Caribbean

Tree Size: 65 ft (20 m) tall, 3-5 ft (1.0-1.5 m) trunk diameter

Average Dried Weight: 42 lbs/ft3 (670 kg/m3)

Basic Specific Gravity: .56

Hardness: 1,160 lbf (5,150 N)

Rupture Strength: 13,520 lbf/in2 (93,230 kPa)

Elastic Strength: 1,385,000 lbf/in2 (9,550 MPa)

Crushing Strength: 7,090 lbf/in2 (48.9 MPa)

Shrinkage: Radial: 3.7%, Tangential: 4.4%, Volumetric: 6.5%, T/R Ratio: 1.2

Color/Appearance: Heartwood color can vary a fair amount with Cuban Mahogany, from a pale pinkish brown, to a darker reddish brown. Typically, the denser the wood, the darker the color. Color tends to darken with age.

Grain/Pore: Has medium to large sized pores, and a medium texture. Grain can be straight, interlocked, irregular or wavy. Mahogany also exhibits an optical phenomenon known as chatoyancy. (See video below.)

Durability: Considered durable or very durable in regards to decay resistance, though it has been reported as being susceptible to insect attack.

Workability: Typically very easy to work with tools: machines well. (With exception to sections with figured grain, which can tearout or chip during machining.) Slight dulling of cutters can occur. Sands very easily. Turns, glues, stains, and finishes well.

Scent: There is no characteristic odor associated with this wood species.

Safety: Although severe reactions are quite uncommon, Cuban Mahogany has been reported as a skin irritant. See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Price/Availability: For the most part, Cuban Mahogany is no longer commercially available. Very small quantities are occasionally made available, which tend to be expensive.

Comments: Historically, perhaps the most celebrated and revered cabinet and furniture wood in the world. Cuban Mahogany has been used extensively in cabinetry and furniture-making for centuries in Europe and the United States, being harvested to the point of complete depletion. Nearly 100 years ago, H.O. Neville wrote of the wood’s exploitation in his 1919 work, Hardwoods of Cuba:

For domestic purposes, the Mahogany is used in such freedom that it seems sacrilege to the newcomer from the North, who has known this wood only in its finished and very expensive forms. Many hundreds of cords of this timber, ranging from 12 inches in diameter down, are annually burned under the boilers of our sugar mills and locomotives: hundreds of trees of the proper sizes are annually cut down and rough-hewed into railroad ties; and for posts, corralled fences, and the myriad other uses of the plantation, Mahogany is utilized. There will come a day not very far distant when the waste of this valuable timber will be regretted.

In 1946, Cuban banned all exporting of the wood due to over-harvesting and high demand; it has also been in scarce supply from other sources in the Caribbean as well. Today, the lumber has become so obscure that the term “Genuine Mahogany” now applies almost exclusively to its close substitute, Honduran Mahogany (Swietenia macrophylla), rather than the Cuban wood that for centuries has simply been referred to as “Mahogany.”

Cuban Mahogany’s easy workability, combined with its beauty and phenomenal stability have made this lumber an enduring favorite. Mahogany is commonly used for: furniture, cabinetry, turned objects, veneers, musical instruments, boat-building, carving, and unfortunately, utility and fuel wood.

Related Species:

Related Articles:

Scans/Pictures: There are currently no pictures of this exact wood species, but a similar species within the Swietenia genus is being substituted (Swietenia macrophylla). If you’d like to contribute a wood sample of this specific species to be scanned, (even small pieces of veneer can be sent), please use the contact form.

Honduran Mahogany (sanded)

Honduran Mahogany (sanded)

Honduran Mahogany (sealed)

Honduran Mahogany (quartersawn)

Honduran Mahogany (fiddleback)

Honduran Mahogany (fiddleback)


Share Your Experience with this Wood Species: