Burma Padauk (Pterocarpus macrocarpus)

Burma Padauk (Pterocarpus macrocarpus)

View More Images Below

Common Name(s): Burma Padauk

Scientific Name: Pterocarpus macrocarpus

Distribution: Myanmar (formerly Burma), and Thailand

Tree Size: 60-80 ft (18-24 m) tall, 2-3 ft (.6-1 m) trunk diameter

Average Dried Weight: 54 lbs/ft3 (865 kg/m3)

Specific Gravity (Basic, 12% MC): .75, .87

Janka Hardness: 2,150 lbf (9,550 N)

Modulus of Rupture: 20,130 lbf/in2 (138.8 MPa)

Elastic Modulus: 2,050,000 lbf/in2 (14.14 GPa)

Crushing Strength: 9,030 lbf/in2 (62.3 MPa)

Shrinkage: Radial: 3.4%, Tangential: 5.8%, Volumetric: 8.4%, T/R Ratio: 1.7

Color/Appearance: Heartwood color can vary, ranging from a pale golden yellow to a deeper reddish brown. Color tends to darken to a golden brown over time. Yellow sapwood is well demarcated from heartwood. Overall, Burma Padauk’s color tends to be less red and more subdued than African Padauk.

Grain/Texture: Grain is usually interlocked, with a coarse texture and fairly large and open pores.

Endgrain: Diffuse-porous; large pores in no specific arrangement; solitary and radial multiples of 2-3; mineral deposits occasionally present; growth rings indistinct; rays not visible without lens; parenchyma diffuse-in-aggregates, aliform (winged), confluent, and banded.

Rot Resistance: Rated as very durable regrading decay resistance, with good resistance to termites and other insects.

Workability: Because of its higher density (as compared to African Padauk), and its interlocked grain, Burma Padauk can be difficult to work with. Burma Padauk turns, glues, and finishes well.

Odor: Padauk has a faint aromatic scent while being worked.

Allergies/Toxicity: Although severe reactions are quite uncommon, Burma Padauk has been reported as a sensitizer. Usually most common reactions simply include eye, skin, and respiratory irritation. See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Pricing/Availability: Available much less often than African Padauk, Burma Padauk is likely to be in the mid to upper range for an imported hardwood.

Sustainability: This wood species is not listed in the CITES Appendices or on the IUCN Red List of Threatened Species.

Common Uses: Veneer, flooring, turned objects, musical instruments, furniture, tool handles, and other small specialty wood objects.

Comments: Burma Padauk is the heaviest and hardest of all types of Padauk (Pterocarpus genus) commercially available. The color tends to be a bit more subdued than the more common African variety.

Related Species:


Burma Padauk (Pterocarpus macrocarpus)

Burma Padauk (sanded)

Burma Padauk (sealed)

Burma Padauk (sealed)

Burma Padauk (endgrain)

Burma Padauk (endgrain)

Burma Padauk (endgrain 10x)

Burma Padauk (endgrain 10x)