Boxwood (Buxus sempervirens)

Boxwood (Buxus sempervirens)

View More Images Below

Common Name(s): Boxwood, Common Box, European Box

Scientific Name: Buxus sempervirens

Distribution: Europe, northwest Africa, and southwest Asia

Tree Size: 10-25 ft (3-8 m) tall, 4-6 in (12-20 cm) trunk diameter

Average Dried Weight: 55 lbs/ft3 (885 kg/m3)

Basic Specific Gravity: .68

Hardness: 2,840 lbf (12,610 N)

Rupture Strength: 20,960 lbf/in2 (144,520 kPa)

Elastic Strength: 2,494,000 lbf/in2 (17,200 MPa)

Crushing Strength: 9,950 lbf/in2 (68.6 MPa)

Shrinkage: Radial: 5.0%, Tangential: 9.0%, Volumetric: 14.0%, T/R Ratio: 1.8

Color/Appearance: Color tends to be a light cream to yellow, which tends to darken slightly with prolonged exposure to light.

Grain/Pore: Boxwood has a fine, even texture with a natural luster. The grain tends to be straight or slightly irregular.

Endgrain: Diffuse-porous; very small pores in no specific arrangement; exclusively solitary; growth rings distinct due to decrease in latewood pore frequency and color change; rays barely visible without lens; parenchyma vasicentric.

Durability: Heartwood is rated as durable, though it can become stained with dark streaks due to fungal attack. Occasionally susceptible to insect attack.

Workability: Boxwood tends to be somewhat difficult to work in flat dimensions, though it is superbly suited for turning. Tearout can occur on pieces with irregular grain during planing and other machining operations. Boxwood has a slight blunting effect on cutters.

Scent: There is no characteristic odor associated with this wood species.

Safety: Although severe reactions are quite uncommon, Boxwood has been reported as a sensitizer. Usually most common reactions simply include eye, skin, and respiratory irritation. See the articles Wood Allergies and Toxicity and Wood Dust Safety for more information.

Price/Availability: Usually only available in small quantities and sizes, Boxwood tends to be very expensive.

Comments: It’s a shame that the term “Boxwood” has become so convoluted and confused in modern times, as there seems to be one particular wood species that has historically been associated with the name Boxwood: Buxus sempervirens. It is this species that can be considered the original, genuine boxwood. Other species in different genera tend to have similar appearances and working characteristics, (i.e., fine texture, hard, and heavy), and perhaps get marketed under the  boxwood name, much like many woods are called by the mahogany name.

Boxwood is well-suited for carving and turning, and the tree’s diminutive size restricts it to smaller projects. Some common uses for Boxwood include: carvings, chess pieces, musical instruments (flutes, recorders, woodwinds, etc.), rulers, handles, turned objects, and other small specialty items.

Related Species:

None available.

Scans/Pictures: A special thanks to Steve Earis for providing the wood sample and turned photo of this wood species.

Boxwood (sanded)

Boxwood (sanded)

Boxwood (sealed)

Boxwood (sealed)

Boxwood (endgrain)

Boxwood (endgrain)

Boxwood (endgrain 10x)

Boxwood (endgrain 10x)

Boxwood (turned)

Boxwood (turned)

Share Your Experience with this Wood Species: